GEt Quote
  • How to Read a Plastics Datasheet: MFR, HDT and Vicat

    Nov 15, 2026 | ACS MATERIAL LLC

    This guide explains how to read a plastics datasheet by checking the test conditions attached to MFR, HDT and Vicat values. A datasheet line such as a melt flow rate, a heat deflection temperature or a Vicat softening temperature looks like a single number, but it is really a result plus the conditions it was measured under. The guide shows what to check beside each of the three lines before two materials are compared, what no single line can tell you, and where each test is explained in detail. It is a reading guide: it prints no values for any material and no pass or fail verdict, and its layouts use placeholders on purpose. The instruments that run these tests are in the Polytevo Series by ACS Material.

    What this guide covers. The three lines most often compared on a plastics datasheet — melt flow, heat deflection temperature and Vicat softening temperature — and the conditions that belong beside each. It does not give limits for any material and it does not say what any value means for a part.
    A sheet of paper with an empty ruled table on a bench, with three small flat plastic specimens and a magnifier
    A datasheet line is a result plus the conditions it was measured under; the conditions decide whether two numbers can be compared.

    1.  How to read a plastics datasheet: start with the conditions

    Each of the three lines answers a different question, and each is incomplete without a few words printed beside it.

    Datasheet lineThe question it answersWhat must be beside the numberDetail guide
    MFR or MVR (melt flow)How readily the melt is pushed through a die at a set temperature and loadMass or volume basis, temperature, loadMFR vs MVR: Melt Flow Rate by Mass and by Volume and Melt Flow Index Test Conditions and Instrument Types
    HDT (heat deflection temperature)The temperature at which a loaded bar has deflected by a set amountMethod letter, heating rate, how the specimen was preparedHDT vs Vicat: Two Softening Temperatures Compared
    VST (Vicat softening temperature)The temperature at which a flat-ended needle has sunk 1 mmMethod code, which includes the heating rateHDT vs Vicat: Two Softening Temperatures Compared

    2.  Reading a melt flow line

    A melt flow line should identify the quantity, test temperature, load and result, for example: MFR ([temperature in °C]/[load in kg]) = [value] g/10 min. The withdrawn edition cited here used this temperature/load notation and asked for two significant figures.1 Check these points in order.

    • Mass or volume. The melt mass-flow rate (MFR) is expressed in g/10 min and the melt volume-flow rate (MVR) in cm³/10 min; the two are not the same number, and the current method says one can be derived from the other only if the melt density at the test temperature is known.2
    • Temperature and load. Both are part of the result. The ASTM method says the flow rate it measures is not a fundamental polymer property but an empirically defined parameter, critically influenced by the conditions of measurement.3
    • A smaller die. The current method defines a standard die and a half-size die, and says use of the half-size die must be stated.2
    • Who set the condition. The conditions are normally specified in the material standard,2 and where a material specification applies, the ASTM method advises reading it first because its modifications take precedence.3

    The arithmetic, the density link and the usual conditions are in MFR vs MVR: Melt Flow Rate by Mass and by Volume and Melt Flow Index Test Conditions and Instrument Types.

    3.  Reading an HDT line

    An HDT line should look like this: HDT, method [letter] = [value] °C, ideally with the heating rate and the specimen preparation beside it. The check list:

    • The method letter. The HDT methods A, B and C use different flexural stresses. Report the method letter with the result; preparation and other test conditions can also affect the value.4
    • What it is. It is the temperature at which a test specimen loaded in three-point bending reaches a standard deflection as the temperature rises.5
    • Comparability. The method says true comparability can only be achieved for materials with the same room-temperature flexural modulus.6
    • Preparation. Annealing generally raises the temperature of deflection, and moulding conditions affect the result.4

    4.  Reading a Vicat line

    A Vicat line should look like this: VST, method [code] = [value] °C. The method code matters because it carries both the force and the heating rate: the methods are named A50, B50, A120 and B120, where the letter selects the force and the number is the heating rate in °C/h, and the test report includes the method code.7

    • The heating rate. For some materials tested, the Vicat method reports values at the higher rate that were up to 10 °C higher than those at the lower rate. This observation is not a conversion rule; reference tests use the lower rate.7
    • The material. The Vicat method applies only to thermoplastics,7 and the ASTM Vicat method is not recommended for materials with a wide Vicat softening range.8

    The side-by-side comparison of HDT and Vicat is in HDT vs Vicat: Two Softening Temperatures Compared.

    5.  What no single line tells you

    • It is not a service temperature. The HDT method says its results do not necessarily represent maximum applicable temperatures and are not intended to predict actual end-use performance.6
    • It is not a processing prediction. The ISO melt flow text notes that its shear rates are much smaller than those under normal processing conditions, so the data may not always correlate with processing behavior.2
    • It does not describe other properties. The ASTM melt flow method says its data indicate the uniformity of the flow rate of a polymer made by an individual process and are not to be used as an indication of uniformity of other properties without valid correlation with other tests.3
    • The two method families are different tests. The ASTM heat deflection method states that results shall not be compared with those of the ISO method.9

    Test method reference: ISO 1133-1:2022 and ASTM D1238-26 for melt flow; ISO 75-1:2020, ISO 75-2:2013 and ASTM D648-18 for heat deflection; ISO 306:2022 and ASTM D1525-25 for Vicat softening temperature.2,3,6,4,9,7,8

    6.  A short checklist before comparing two datasheets

    1. Is each value from the same test and the same basis (mass or volume; the same HDT method letter; the same Vicat method code)?
    2. Were the conditions the same: the same temperature and load for melt flow, the same heating rate for HDT and Vicat?
    3. Does the datasheet say which edition of the method was used, and how the specimens were prepared?
    4. Is the number a typical value or a specification limit? Check whether the datasheet identifies which it is.

    7.  Where the Polytevo Series instruments fit

    The page values below are quoted as published. They are not datasheet values for any material, and this guide does not say that either instrument realises a particular method.

    The Polytevo Series Melt Flow Indexer page describes the ACS-5005 series as determining the melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of plastics and resins in the viscous flow state at a set temperature and load, in three configurations: the standard ACS-5005, the automatic ACS-5005A and the ACS-5005SA with motorized lifting and lowering of the load weights.

    The Polytevo Series HDT and Vicat Softening Temperature Tester page describes the ACS-5006-TC3 as a three-station heat deflection temperature (HDT) and Vicat softening temperature (VST) tester with a temperature range of RT to 300°C, two selectable heating rates, a 25 L oil bath and computer-controlled operation.

    The supplied configuration is confirmed on the quotation.

    8.  Where to go next

    For the way melt flow and heat tests fit into a lab-scale route from material to test, start with the Lab-Scale Polymer Processing and Testing: A Workflow Guide. For the melt flow line, read MFR vs MVR: Melt Flow Rate by Mass and by Volume and then Melt Flow Index Test Conditions and Instrument Types; for HDT and Vicat, read HDT vs Vicat: Two Softening Temperatures Compared; for strength, toughness and hardness lines, read Mechanical Testing of Plastics: Match the Test to the Question.

    9.  Keep Exploring the Lab-Scale Polymer Processing Knowledge Hub

    This guide belongs to the ACS Material library on lab-scale polymer processing and testing, built around the Polytevo Series by ACS Material. Start from the Lab-Scale Polymer Processing and Testing: A Workflow Guide, which places every stage of the work, from material to test, on one route. The other guides on melt flow and heat tests are:

    • MFR vs MVR: Melt Flow Rate by Mass and by Volume (coming soon) — how melt mass-flow rate and melt volume-flow rate are defined, and the arithmetic that links them.
    • Melt Flow Index Test Conditions and Instrument Types (coming soon) — what a melt flow test condition contains, and how the three indexer configurations differ.
    • HDT vs Vicat: Two Softening Temperatures Compared — what each softening temperature measures, and which question each one answers.

    10.  Before you request a quote

    To help identify a suitable configuration, describe the tests behind the datasheet lines you need. Please tell us:

    • which tests you run: melt flow, HDT, Vicat or a combination;
    • the materials you test and the form of the specimens;
    • the temperature range you expect to reach;
    • how many specimens you run at a time;
    • your mains supply.

    Send these through Request a Quote. Specifications are as published on each product page, and final configurations are confirmed on quotation.

    11.  FAQ

    Can I compare two MFR values from different datasheets?

    For a like-for-like comparison, check that both results are MFR and identify the method and edition, temperature, load, die and relevant sample preparation. Matching temperature and load alone does not establish that the measurements were obtained in equivalent conditions.2,3

    Is a higher HDT always better?

    The HDT method says its results do not necessarily represent maximum applicable temperatures and are not intended to predict end-use performance, so a higher value does not by itself say what a part will tolerate.6

    Why does a Vicat value carry a code such as A50 or B120?

    The letter selects the force and the number is the heating rate in °C/h, and the test report includes the method code.7

    Can I compare HDT and Vicat values with each other?

    They measure different things, a deflection under bending load and a 1 mm penetration, so they are read each against its own method.5,7

    12.  References

    1Test method reference: ISO 1133:1997. Plastics — Determination of the melt mass-flow rate (MFR) and the melt volume-flow rate (MVR) of thermoplastics. Third edition, 1997; a withdrawn edition. Public preview copy read for this guide: Source record
    2Test method reference: ISO 1133-1:2022. Plastics — Determination of the melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of thermoplastics — Part 1: Standard method. Source record
    3Test method reference: ASTM D1238-26. Standard Test Method for Melt Flow Rates of Thermoplastics by Extrusion Plastometer. Source record
    4Test method reference: ISO 75-2:2013. Plastics — Determination of temperature of deflection under load — Part 2: Plastics and ebonite. Source record
    5Test method reference: ISO 75-1:2013. Plastics — Determination of temperature of deflection under load — Part 1: General test method. Third edition, 2013; superseded by the 2020 edition. Public preview copy read for this guide: Source record
    6Test method reference: ISO 75-1:2020. Plastics — Determination of temperature of deflection under load — Part 1: General test method. Source record
    7Test method reference: ISO 306:2022. Plastics — Thermoplastic materials — Determination of Vicat softening temperature (VST). Source record
    8Test method reference: ASTM D1525-25. Standard Test Method for Vicat Softening Temperature of Plastics. Source record
    9Test method reference: ASTM D648-18. Standard Test Method for Deflection Temperature of Plastics Under Flexural Load in the Edgewise Position. Source record
    Disclaimer: This guide provides general information based on the cited sources and dated product-page snapshots. ACS Material makes no representations or warranties, either express or implied, regarding the suitability of any Polytevo Series product for any particular purpose or the accuracy of the information listed here. Product statements are those published on the Polytevo Series product pages on 15 November 2026; specifications are as published on each page and final configurations are confirmed on quotation. Literature statements are those of the cited authors and were not produced with Polytevo Series equipment unless the source says so. Standards are named only as test method references; this guide makes no claim about the standards status of any product. Always follow the method reference, the product documentation and your laboratory’s safety procedures.